Material No.: 1.4571

Material data for 1.4571

The material 1.4571 is a rust and acid-resistant stainless steel with the abbreviation X6CrNiMoTi17-12-2. In the American ASME standard, it has the designation UNS S31635.

How far does the scope of the information listed here extend?

The data below applies to hot-rolled and cold-rolled sheet and strip from our product range.

The information given here on properties/usability is not a guarantee of properties, but is for descriptive purposes only. The information is provided for advisory purposes and is based on information from the standards/sources: DIN EN 10088-2, DIN EN 10028-7, AD 2000 W2/W10, ASME code SA240/480, reference book Steel Code.

We cannot accept any liability for the information or the results of processing/application.

What are other designations for 1.4571?

ASME (incl. double attestation): SA240 316Ti

EN (incl. double attestation): 1.4571

How is the material 1.4571 heat-treated and processed?

Temperature: 1,030-1,110 °C
Cooling methods: Water, air
Microstructure: austenitic
Microstructure Polishable: no
Possible welding processes: Gas-shielded welding, arc welding, resistance welding (gas fusion welding or autogenous welding) (limited)

 

 

 

 

 

 

Chemical Composition:

(in accordance with EN 10088-2, ASME SA240 incl. the above-mentioned double attestations)

  C Si Mn P S Cr Ni Mo Ti N
min           16,500 10,500 2,000    
max 0,080 0,750 2,000 0,045 0,015 18,000 13,500 2,500 0,700 0,100

Values in %

Mechanical properties at room temperature:

(in the solution-annealed state)

The values below take into account the above-mentioned double attestations. Limit values from EN 10088-2, EN 10028-7, AD 2000 W2/W10 and according to ASME SA240/480.

C = cold-rolled strip; H = hot-rolled strip; P = plate

In accordance with AD 2000 regulations, the KBZ is only carried out and confirmed in the certificate for thicknesses > 20 mm.

    Yield strength Tensile Strength Elongation at break Notch impact energy (ISO-V)
Product form Thickness [mm] max Rp0,2 Rp1,0 Rm A5 A50 ≥ 10 mm Thickness
    [N/mm2] min [N/mm2] [%] min [%] min [J] transverse
C 8 240 270 520–720 40 40 60
H 13,5 220 260 520–720 40 40 60
P 75 220 240 515–700 40 40 60

Physical properties:

Density
at 20 °C
Modulus of elasticity
at 20 °C
Specific heat capacity
at 20 °C
Thermal conductivity
at 20 °C
Electrical resistance
at 20 °C
kg/dm3 GPa J / g x K W / K x m Ω x mm2 / m
8 200 0,50 15 0,75

Field of application

Pipeline construction, construction industry, apparatus engineering, chemical industry, food industry, mechanical engineering, medical and pharmaceutical industry, shipbuilding, textile industry, rubber industry. As delivered, the steel is resistant to intergranular corrosion (e.g. ASTM A262 Pr. E / EN 3651-2); in the welded condition, resistance is also guaranteed by the titanium alloy.

  • 1.4571 This data sheet applies for hot and cold rolled sheets and strips from our stock.

Any Questions?